UNIVERSITY OF HELSINKI REPORT SERIES IN PHYSICS HU-P-D135 A STUDY OF THE NANOSTRUCTURE OF THE CELL WALL OF THE TRACHEIDS OF CONIFER XYLEM BY X-RAY SCATTERING Seppo Andersson Division of X-ray Physics Department of Physical Sciences Faculty of Science University of Helsinki Helsinki, Finland ACADEMIC DISSERTATION To be presented, with the permission of the Faculty of Science of the University of Helsinki, for public criticism in Auditorium B123 of Exactum, Gustaf Hällströmin katu 2b, on 12th January 2007, at 12 o’clock. Helsinki 2006 Report Series in Physics HU-P-D135 ISBN 952-10-3234-0 ISSN 0356-0961 ISBN 952-10-3235-9 (pdf) http://www.ethesis.helsinki.fi Helsinki 2006 Yliopistopaino 1 Preface This thesis is based on research done at the Division of X-ray Physics, the Department of Physical Sciences, University of Helsinki, in collaboration with the Finnish Forest Research Institute (METLA), the Laboratory of Polymer Chemistry, Department of Chemistry, University of Helsinki, and the Technical Research Centre of Finland (VTT). I wish to thank Professor Juhani Keinonen, the head of Department of Physical Sciences, for the opportunity to work at the Department of Physical Sciences as an amanuensis at the Physics Teacher Education Unit and at the same time to do my doctoral thesis at the Division of X-ray Physics. Professors Seppo Manninen and Keijo Hämäläinen, as heads of the Division of X-ray Physics, I wish to thank for placing the facilities at my disposal and the pleasant and stimulating working atmosphere. I also wish to thank Professor Heimo Saarikko, the head of the Physics Teacher Education Unit, for understanding and encouraging attitude to my research work at the Division of X-ray Physics. I wish to express my deepest gratitude to my supervisor, Professor Ritva Serimaa, for her guidance and patience during these years and for critical comments of the manuscript. I wish to thank Professor emeritus Timo Paakkari - without him, I would have never started to study wood by means of x-ray scattering. In addition, I wish to thank Doc. Pekka Saranpää for inspirational discussions. I am grateful to research partners: Professor Sirkka Liisa Maunu and Dr. Hanne Wikberg for the NMR spectroscopic measurements, Professor Pertti Viitaniemi and MSc Saila Jämsä for the thermally modified wood samples, Doc. Pekka Saranpää, Lich.Phil. Erkki Pesonen, and Mr. Tapio Järvinen for providing the wood samples, Dr. Tuuli Timonen and MSc Pirkko Harju (Botanical Museum, Univ. of Helsinki) for the SEM images. I am grateful to former and current researchers at the Division of X-ray Physics: Dr. Matti Sarén, MSc Marko Peura, MSc Simo Siiriä, and MSc Tiina Väänänen for assisting in the WAXS experiments, Dr. Mika Torkkeli and MSc Ulla Vainio for assisting the SAXS experiments, Dr. Kaija Jokela, Dr. Veli Eteläniemi, Dr. Manuel Fernández, and MSc Teemu Ikonen conducting the USAXS measurements at the Hamburger Synchrotronstrahlungslabor (HASYLAB), Germany. In addition, I wish to thank Dr. Kaija Jokela for assisting in data analysis. I am grateful to Doc. Merja Blomberg, MSc Matti Laitinen, Mr. Pekka Pihkala, and MSc Marko Peura for helping me in technical problems regarding to powder diffractometers and x-ray generators. I am also grateful to personnel at the Physics Teacher Education Unit. I wish to mention Doc. Ismo Koponen, Dr. Ari Hämäläinen, and MSc Ilkka Hendolin for understanding and encouraging attitude to my research work. Finally, I want to thank my parents and brothers for their caring and support. The financial support of Jenny and Antti Wihuri Foundation is gratefully acknowledged. November, 2006 Seppo Andersson 2 S. Andersson: A Study of the Nanostructure of the Cell Wall of the Tracheids of Conifer Xylem by X-Ray Scattering, University of Helsinki, 2006, 39 pages + appendices. University of Helsinki, Report Series in Physics, HU-P-D135, ISBN 952-10-3234-0, ISSN 0356-0961, ISBN 952-10-3235-9 (pdf). Classification: (INSPEC): A6110F, A6140K, A8140G;(CABICODES): FF030, FF040, KK510, KK520, ZZ900 Keywords: x-ray scattering, xylem, cellulose crystallite, crystallinity, microfibril angle, Picea abies, Pinus sylvestris, thermally modified wood Abstract The purpose of this study was to develop practical and reliable x-ray scattering methods to study the nanostructure of the wood cell wall and to use these methods to systematically study the nanostructure of Norway spruce and Scots pine grown in Finland and Sweden. Methods to determine the microfibril angle (MFA) distribution, the crystallinity of wood, and the average size of cellulose crystallites using wide-angle x-ray scattering were developed and these parameters were determined as a function of the number of the year ring. The mean MFA in Norway spruce decreases rapidly as a function of the number of the year ring and after the 7th year ring it varies between 6° and 10°. The mean MFA of Scots pine behaves the same way as the mean MFA of Norway spruce. The thickness of cellulose crystallites for Norway spruce and Scots pine appears to be constant as a function of the number of the year ring. The obtained mean values are 32 Å for Norway spruce and 31 Å for Scots pine. The length of the cellulose crystallites was also quite constant as a function of the year ring. The mean length of the crystallites for Norway spruce was 364 Å, while the standard deviation was 27 Å. The mass fraction of crystalline cellulose in wood is the crystallinity of wood and the intrinsic crystallinity of cellulose is the crystallinity of cellulose. The crystallinity of wood increases from the 2nd year ring to the 10th year ring from the pith and is constant after the 10th year ring. The crystallinity of cellulose obtained using nuclear magnetic resonance spectroscopy was 52% for both species. The crystallinity of wood and the crystallinity of cellulose behave the same way in Norway spruce and Scots pine. The methods were also applied to studies on thermally modified Scots pine wood grown in Finland. Wood is modified thermally by heating and steaming in order to improve its properties such as biological resistance and dimensional stability. Modification temperatures varied from 100 °C to 240 °C. The thermal modification increases the crystallinity of wood and the thickness of cellulose crystallites but does not influence the MFA distribution. When the modification temperature was 230 °C and time 4 h, the thickness of the cellulose crystallites increased from 31 Å to 34 Å. 3 Contents Preface ...................................................................................................................................1 Abstract..................................................................................................................................2 List of papers..........................................................................................................................4 Author’s contribution .............................................................................................................5 1 Introduction ....................................................................................................................6 1.1 Structure and chemistry of wood.............................................................................6 1.2 X-ray diffraction as tool to study wood structure.....................................................8 2 Samples ..........................................................................................................................8 3 The cellular structure of softwood...................................................................................9 4 X-ray scattering from softwood.....................................................................................12 5 WAXS measurements...................................................................................................16 5.1 Microfibril angle ...................................................................................................16 5.2 Crystallinity ..........................................................................................................16 5.3 The size of cellulose crystallites ............................................................................16 6 Data analysis.................................................................................................................18 6.1 The determination of the microfibril angle ............................................................18 6.2 The determination of the crystallinity....................................................................19 6.3 The determination of the average size of cellulose crystallites...............................20 7 Results..........................................................................................................................21 7.1 Norway spruce and Scots pine grown in southern Finland .....................................21 7.2 Irrigated and fertilized Norway spruce grown in southern Sweden ........................21 7.3 Thermally modified Scots pine grown in Finland ..................................................22 8 Discussion ....................................................................................................................23 9 Conclusions ..................................................................................................................28 10 References ................................................................................................................29 4 List of papers This thesis consists of an introductory part followed by five research papers. The papers are referred to by Roman numerals I - V throughout the text. The papers are reproduced with the kind permission of the journals concerned. I Andersson S., Serimaa R., Torkkeli M., Paakkari T., Saranpää P., Pesonen E. (2000) Microfibril angle of Norway spruce [Picea abies (L.) Karst.] compression wood: comparison of different measuring techniques. Journal of Wood Science 46 (5): 343-349. II Sarén M-P., Serimaa R., Andersson S., Paakkari T., Saranpää P., Pesonen E. (2001) Structural variation of tracheids in Norway Spruce (Picea abies [L.] Karst.). Journal of Structural Biology 136 (2): 101-109. III Andersson S., Serimaa R., Paakkari T., Saranpää P., Pesonen E. (2003) Crystallinity of wood and the size of cellulose crystallites in Norway spruce (Picea abies ). Journal of Wood Science 49 (6): 531-537. IV Andersson S., Wikberg H., Pesonen E., Maunu S.L., Serimaa R. (2004) Studies of crystallinity of Scots pine and Norway spruce cellulose. Trees - Structure and Function 18: (3): 346-353. V Andersson S., Serimaa R., Väänänen T., Paakkari T., Jämsä S., Viitaniemi P. (2005) X-ray scattering studies of thermally modified Scots pine (Pinus sylvestris L.). Holzforschung 59 (4): 422-427. 5 Author’s contribution Paper I This work has been done in collaboration with the Finnish Forest Research Institute (METLA), Vantaa Research Unit. The sample was prepared at METLA. X-ray scattering studies were carried out at the Division of X-ray Physics, Department of Physical Sciences, University of Helsinki. The author was responsible for the WAXS experiments and Mika Torkkeli was responsible for the SAXS experiments. Pekka Saranpää and Erkki Pesonen were responsible for polarizing microscopy measurements. Paper II This work has been done in collaboration with METLA, Vantaa Research Unit. The samples were prepared at METLA. X-ray scattering studies were carried out at the Division of X-ray Physics, Department of Physical Sciences, University of Helsinki. The author was responsible for the WAXS experiments and the WAXS data analysis. In addition, Simo Siiriä and Matti Sarén assisted in the WAXS experiments. Matti Sarén was responsible for measurements and data analysis regarding the shape and size of the cell cross-section and the thickness of the cell wall. Paper III This work has been done in collaboration with METLA, Vantaa Research Unit. The samples were prepared at METLA. X-ray scattering studies were carried out at the Division of X-ray Physics, Department of Physical Sciences, University of Helsinki. The author was responsible for the WAXS experiments and the WAXS data analysis. Paper IV This work has been done in collaboration with the Laboratory of Polymer Chemistry, Department of Chemistry, University of Helsinki, and METLA, Vantaa Research Unit. The samples were prepared at METLA. X-ray scattering studies were carried out at the Division of X-ray Physics, Department of Physical Sciences, University of Helsinki. NMR spectroscopic measurements were carried out at the Laboratory of Polymer Chemistry. The author was responsible for the WAXS experiments and the WAXS data analysis. Hanne Wikberg was responsible for the NMR spectroscopic measurements. Paper V This work has been done in collaboration with the Technical Research Centre of Finland (VTT), Building and Transport. The samples were prepared at VTT. X-ray scattering studies were carried out at the Division of X-ray Physics, Department of Physical Sciences, University of Helsinki. The author was responsible for the WAXS experiments and the WAXS data analysis. Kaija Jokela, Veli Eteläniemi, Manuel Fernández and Teemu Ikonen conducted the USAXS measurements at the Hamburger Synchrotronstrahlungslabor (HASYLAB), Germany. 6 1 Introduction 1.1 Structure and chemistry of wood A tree is a perennial tall-growing woody plant. It is self-supporting with roots, a solid trunk and a crown (Bernatzky, 1978). The roots keep the tree standing upright in the soil and also serving to collect water and nutrients from the soil. Figure 1 presents sections of the trunk. The xylem (wood) is organized in concentric year rings around the pith. The inner part is dead heartwood and the outer part is sapwood, in which ascent of the sap takes place. Cambium, which is between the phloem (inner bark) and the xylem, each year produces new xylem and phloem cells. Outside the phloem is the outer bark (Sjöström, 1993). Fig. 1 Sections of the trunk (Sjöström, 1993). The xylem provides structural support for a tree. The xylem and the phloem make up the vascular systems found contiguously in the roots, stems and leaves of plants (Nobel, 1999). Water and nutrients are transported via the outermost annual rings of the xylem from the roots to elsewhere in the tree, especially to the leaves and needles, where photosynthesis occurs. The xylem consists of tubular elongated cells. Conifer tracheids are connected to each other with bordered pits. In photosynthesis, carbon dioxide (CO2) and water (H2O) transform to oxygen (O2) and glucose (C6H12O6) according to the chemical equation: 6 CO2 + 6 H2O : 6 O2 + C6H12O6. Glucose, which is the basis for other organic compounds like cellulose, is transported from the leaves to other parts of the tree via the phloem (Bernatzky, 1978). Both cell division and the radial growth of the tree take place in the cambium (Sjöström, 1993). A softwood cell has a lumen the diameter of which is about 30-35 µm in earlywood and 20 µm in latewood (Wagenführ and Scheiber, 1989, Paper II). In radial cell walls of 7 earlywood there are bordered pit pairs the diameter of which varies from 10 µm to 20 µm. In latewood there are also bordered pit pairs in the tangential cell walls (Fagerstedt et al., 1996). The wood cell wall has a complex multilayer nanostructure in which cellulose molecules are grouped together in partially crystalline microfibrils embedded in a matrix composed of lignin and hemicelluloses. The physical properties of Norway spruce and Scots pine have been studied extensively. The behaviour of the basic density of Norway spruce and Scots pine differs from each other in the radial as well as the longitudinal direction. The density of Scots pine increases as a function of the number of the year ring by reaching the maximum near the 80th year ring, while the density of Norway spruce at first decreases and after a few year rings the density begins to increase by reaching the maximum later than Scots pine (Hakkila, 1966). The density of Scots pine decreases as a function of the height, while the density of Norway spruce at first decreases as height increases, but from the middle of the stem the density begins to increase (Hakkila, 1966). The length of tracheids in Norway spruce and Scots pine increases as a function of the number of the year ring (Saranpää, 1994; Lindström, 1997; Fries et al., 2003). It is well known that the strength properties vary in different stem directions. For example, wood is 4 to 12 times stronger in compression, parallel to the fibre axis than it is perpendicular to the fibre axis (Panshin and de Zeeuw, 1980). Kennedy (1995) has shown that the longitudinal MOE increases as a function of the year ring for Tsuga heterophyla. The longitudinal stiffness modulus of Norway spruce increases from 6 GPa to 8.5 GPa, while in the radial and tangential direction the stiffness modulus is nearly constant, 1 GPA and 0.35 GPa (Koponen et al., 2005). The negative correlation between the longitudinal MOE and the orientation of microfibrils has been demonstrated in several publications (e.g. Cave and Walker, 1994; Keckes et al., 2003). Norway spruce Scots pine Juvenile wood Mature wood Juvenile wood Mature wood Longitudinal MOE (MPa) 11 800 13 800 10 000 13 100 Longitudinal MOR (MPa) 76 88 71 94 Weight density (kg/m3) 459 481 445 515 Table 1. Longitudinal modulus of elasticity (MOE), longitudinal modulus of rupture (MOR) and density for Norway spruce and Scots pine grown in southern Finland are presented for both juvenile and mature wood according to Verkasalo and Leban (2002). Weight density is determined at 12% moisture content. Values are rounded. Verkasalo and Leban (2002) studied the longitudinal modulus of elasticity (MOE) and modulus of rupture (MOR) of Norway spruce and Scots pine grown in southern Finland and north-eastern France. In Table 1 the values of MOE, MOR and density for Norway spruce and Scots pine grown in southern Finland are presented for both juvenile wood and mature wood 8 (Verkasalo and Leban, 2002). Weight density was determined at 12% moisture content by measuring the mass and the volume of wood samples. The elastic and shrinkage properties of softwood are successfully modelled based on the cellular structure of wood and properties of the cell walls (e.g. Koponen et al., 1989 and 1991; Astley et al., 1998; Harrington et al., 1998). The elastic properties of single wood fibers are also modelled on by using the structural and chemical properties of the cell wall layers (e.g. Salmén and de Ruvo, 1985; Bergander and Salmén, 2002). 1.2 X-ray diffraction as tool to study wood structure The wavelength of x-ray radiation is suitable for studying the nanostructure of wood. The parameters, which can be determined by using x-ray scattering, include the mean microfibril angle, crystallinity of wood, the specific surface, and the size of cellulose crystallites. The microfibril angles of Norway spruce and Scots pine grown in Finland have been studied earlier but not systematically as a function of the number of the year ring (Kantola and Seitsonen, 1961; Kantola and Kähkönen, 1963; Kantola et al., 1966; Kantola and Seitsonen, 1969; Paakkari and Serimaa, 1984). The purpose of this study was to develop methods to determine the mean microfibril angle (Paper I), the crystallinity of wood (Paper III), and the average size of cellulose crystallites (Paper III). Furthermore, the mean microfibril angle, the crystallinity of wood and the size of cellulose crystallites were determined as a function of the number of the year ring in Norway spruce and Scots pine grown in Finland (Papers II, III and V). Some preliminary results of the determination of the microfibril angle for Norway spruce grown in Finland were presented in Saranpää et al. (1998). The methods were also applied to studies on thermally modified Scots pine wood grown in Finland (Paper V). In this thesis, the length of cellulose crystallites for fertilized and irrigated Norway spruce grown in Sweden was studied. 2 Samples The samples were thin slices of wood or powdered wood. The dimensions of the slices were about 1.0 mm in the radial direction (sample thickness), 15 mm in the tangential direction and 15 mm in parallel to the cell axis. Powdered samples were prepared by cutting match-stick size wood pieces (ca. 1 g), which were milled (Analytical mill A-10, Kinematica, Switzerland) to fine wood powder in 60 seconds. Heating of the sample was avoided by cooling the mill -30 ºC. For the X-ray measurements wood powder (ca. 0.1 g) was pressed into the shape of a tablet, whose diameter was 15 mm with a thickness of 1.0 mm. All samples were earlywood. The Norway spruce samples, which were studied in Papers II, III and IV, were taken from four stems grown in Ruotsinkylä in Finland (lat 60.37° N, long 24.98° E). The age of these trees was about 60 years and the height of these trees was about 24 m. Scots pine samples were studied in Paper IV. These samples were taken from one stem grown in Hyytiälä in Finland (lat 61.84° N, long 24.30° E). The age of this tree was about 40 years with a height of about 20 m. The samples contained neither compression wood nor external damages like cracks or resin pockets. The samples were taken at a height of 1.3 m 9 and both from juvenile and mature wood. These samples were stored several months in normal room conditions before x-ray scattering experiments. In this thesis the influence of fertilization and irrigation on the length of cellulose crystallites were studied. Samples were taken from the fertilized and irrigated Norway spruce stems grown in Asa in southern Sweden (lat 57.13º N, long 14.75º E) (Lundgren 2003). All samples were taken at a height of 1.3 m and both from juvenile and mature wood. Thermally modified Scots pine was also studied (Viitaniemi et al., 1994; Viitaniemi et al., 1995; Sivonen et al., 2002; Nuopponen et al., 2003; Paper V). The source material, the shield gas, the modification times and temperatures are tabulated in Table 2.The source material was kiln-dried or green wood. The kiln-dried wood means green wood, which has been dried at a temperature of 60 ºC for 8 days (192 h). At this temperature of 60ºC, the modification was carried out in air-atmosphere; otherwise, saturated steam was used as a shield gas. Reference samples were prepared from kiln-dried wood. All samples were taken from mature wood, from a year ring number larger than 10. In the case of 4 hours modification time, the samples and their reference samples were taken from the same year ring. Source material Shield gas Modification time (h) Modification temperatures (ºC) kiln-dried wood saturated steam 3 100, 120, 140, 160, 180, 200, 220, 240 kiln-dried wood saturated steam 4 180, 230 green wood saturated steam 48 115 green wood (control samples) air 192 60 Table 2. The source materials, the shield gases, the modification times and temperatures of the thermal modification. 3 The cellular structure of softwood The tissue of softwood is composed of tracheids (90-95%) and ray cells (5-10%) (Sjöström 1993). The tracheids give the mechanical strength and take part in water transport, i.e. the ascent of sap. The cell wall consists of the primary wall and the secondary wall (Fig. 2). The secondary wall consists of several layers of which the S2 layer is the thickest (Tang, 1973; Abe et al., 1991). Between the individual cells, there is a thin layer, the middle lamella, which glues the cells together to form the tissue (Fengel and Wegener, 1984). 10 Fig. 2 The cross-section of a wood cell and middle lamella between the individual cells (Sjöström, 1993). Fig. 3. Cellulose chains form crystalline and amorphous regions in a matrix of amorphous hemicelluloses and lignin. The diameter and the length of the crystalline regions (cellulose crystallites) are 30 Å and 300 Å, respectively. In the unit cell of cellulose I the cellulose chains are parallel to the lattice vector c and perpendicular to the lattice vector a . The cell wall consists mainly of cellulose, hemicellulose and lignin (Sjöström, 1993). Cellulose is synthesized by a rosette (Cosgrove, 2005), which consists of a set of enzymes called cellulose synthases (CESAs). CESAs polymerise glucose molecules into cellulose chains or more exactly into (1,4)-linked  -D-glucan chains (Mauseth, 2003). The length of these chains is at least 5000 nm corresponding to a chain of about 10000 glucose units (Sjöström, 1993). The cellulose chains produced by a rosette form a bunch (Cosgrove, 2005). These bunches are called cellulose microfibrils. Cellulose microfibrils have both amorphous and crystalline regions (crystallites). The diameter of the cellulose microfibrils is the same order of magnitude as the diameter of the cellulose crystallites. 11 As early as 1913, Nishikawa discovered using x-ray scattering that cellulose in fibrous substances, such as wood, bamboo and hemp, has a crystalline structure (Inagaki, 1989). Parallel cellulose chains form crystalline regions (Fig.3). Meyer and Misch (1937) determined the unit cell of native cellulose (cellulose I) from ramie samples for the first time. Atalla and VanderHart (1984) found, using NMR spectroscopy, that native cellulose (cellulose I) is a composite of two distinct crystalline forms: cellulose I. and cellulose I . Cellulose I. has one chain triclinic unit cell and I two-chain monoclinic cell (Sugiyama et al., 1991; Nishiyama et al., 2002; Nishiyama et al., 2003). The relative amounts of the two crystalline forms have been found to vary between samples of different origins (Nishiyama et al., 2003). Cellulose, which is algal or bacterial in origin, is I. rich and cellulose from cotton, wood and ramie fibres is I rich (Nishiyama et al., 2003). In the unit cell of cellulose I the cellulose chains are parallel to the lattice vector c and perpendicular to the lattice vector a . The thickness of cellulose crystallites in a few softwood species has been determined using x- ray scattering (Marton et al. 1972; Nomura and Yamada 1972; Tanaka et al. 1981; Jakob et al., 1995). Marton et al. (1972) studied Norway spruce grown in Syracuse (New York, USA) and Jakob et al. (1995) studied Norway spruce grown in Austria. Nomura and Yamada (1972) and Tanaka et al. (1981) studied one pine species, Pinus densiflora. The results for the thickness of cellulose crystallites varied between 25 Å and 36 Å. Papers III and IV present the thickness of cellulose crystallites for Norway spruce grown in Finland and Paper IV presents the results for Scots pine grown in Finland. The cellulose synthesis is not fully known but one can gather information for it using different methods. Donaldson and Singh (1998) used transmission electron microscopy (TEM) to study transverse sections of the S2 layer and observed that the average diameter of cellulose microfibrils is 36 Å and the majority of microfibrils occur in bundles. The diameter of the microfibril bundles is between 200 Å and 400 Å. The bundles occur randomly in the radial direction of the tracheids, but are present more or less concentrically (Singh and Daniel, 2001). The microfibrils are oriented helically around the fibre axis (Sisson, 1935). The helix can be either left-handed (S helix) or right-handed (Z helix) (Sjöström, 1993). The angle between the microfibrils and the fibre axis is the microfibril angle (MFA). The MFA, in turn, depends on the cell wall layer (Tang, 1973; Abe et al., 1991). Conventional techniques like viewing the pit angle apertures and using polarising microscopy have been used for measuring microfibril angles (Leney, 1981; Donaldson, 1991). However, only a limited number of pits can be measured using that method. To produce statistically better results, x-ray scattering methods have been used. By means of x-ray scattering the average microfibril angles of all wood cell wall layers can be determined simultaneously (Cave, 1966; Sobue et al., 1971; Boyd, 1977; Paakkari and Serimaa, 1984). The MFA of Norway spruce has been studied as a function of the number of the year ring (Sahlberg et al., 1997; Lichtenegger et al., 1999). Peura et al. (2005) studied single wood cell walls by synchrotron x-ray microdiffraction and polarised light microscopy, and these two methods gave very different results for the MFA when measured from the same position of the cell. The former method measures the orientation of cellulose crystallites, whereas the signal in the latter method arises from a far more diverse origin (Peura et al., 2005). 12 4 X-ray scattering from softwood Because solid oriented wood samples have fibre texture, it is possible to get different information about the structure of the cell wall by using different measuring geometries. Figures 4, 5 and 6 present three measuring geometries, which are applied to x-ray scattering studies from softwood. Fig. 4 The perpendicular transmission geometry for determination of the orientation of microfibrils. Fig. 5 The symmetrical transmission geometry for determination of the length of cellulose crystallites and the orientation of microfibrils. Fig. 6 The symmetrical reflection geometry for determination of the diameter of cellulose crystallites. Figure 4 presents the perpendicular transmission geometry, Figure 5 the symmetrical transmission geometry and Figure 6 the symmetrical reflection geometry. The unit vectors 0S and S indicate the directions of the incident and scattered rays. The scattering vector k is also marked. The magnitude of the scattering vector θλpi sin)2(k = , where θ is half of the scattering angle and λ is the wavelength. In most of the studies of this thesis, the tangential face of the wood samples is exposed to the x-ray beam. The fibre axis is parallel to the tangential face. 13 Figure 7 presents the WAXS pattern of a single fibre of Norway spruce, which was measured using the perpendicular transmission geometry (Fig. 4). The Miller indexes of five reflections of cellulose have been marked. Because the cellulose crystallites are oriented almost parallel to the fibre axis (fibre texture), the reflections hkl appear as spots instead of Debye rings. Fig. 7 X-ray diffraction pattern of a Norway spruce single fibre sample measured using perpendicular transmission geometry (ESRF Annual Report 2004). Fibre axis is vertical. Five reflections of cellulose, scattering vector k and azimuthal angle φ are marked. Figures 8 - 12 present x-ray scattering patterns of a control sample of Norway spruce from the 14th year ring. Figure 8 demonstrates the SAXS pattern of the control sample measured using the perpendicular transmission geometry (Fig. 4). Fig. 8 The SAXS pattern of a Norway spruce sample from the 14th year ring measured using perpendicular transmission geometry. The measuring setup is presented in Vainio et al. (2004). The fibre axis is vertical. 14 Figures 9 and 10 represent the WAXS patterns of the control sample measured using the symmetrical transmission geometry with the setup described later in section 7.3. In the case of Figure 9 the fibre axis was vertical (angle φ = 90°) and in the case of Figure 10 the sample had been turned 90° and the fibre axis was horizontal (angle φ = 0°). In the former case, the fibre axis is perpendicular to the scattering vector and equatorial reflections, like the reflection 200, are seen but meridional reflections, like the reflection 004, are not. In the latter case the fibre axis is parallel to the scattering vector and meridional reflections are seen but equatorial reflections are not. In the case of symmetrical reflection geometry, the fibre axis is perpendicular to the scattering vector. Thus, equatorial reflections are seen and meridional reflections are not and the WAXS pattern is similar to the pattern that is presented in Figure 9. Fig. 9 The WAXS pattern of a Norway spruce sample from the 14th year ring measured using symmetrical transmission geometry. The fibre axis is vertical (angle φ = 90°). Fig. 10 The WAXS pattern of a Norway spruce sample from the 14th year ring measured using symmetrical transmission geometry. The fibre axis is horizontal (angle φ = 0°). The reflection 004 in Figure 10 is narrower than the reflection 200 in Figure 9 indicating that the crystallites are longer in the chain direction than in the direction [200]. Amorphous regions also provide a contribution to the WAXS pattern. It is seen as the amorphous background in Figure 9. WAXS is a well-established method for determination of the average size of the crystallites and the crystallinity, i.e. the mass fraction of crystalline material in the sample (Ruland, 1961; Alexander, 1969; Vonk, 1973; Vonk and Fagherazzi 1983; Baltá-Calleja and Vonk, 1989). The mass fraction of crystalline cellulose in wood is the crystallinity of wood and the intrinsic crystallinity of cellulose, in turn, is the crystallinity of cellulose. The fibre texture and the complex chemical composition of wood complicate the crystallinity determination. Furthermore, the separation of amorphous background from the diffraction pattern of cellulose crystallites is difficult because the cellulose crystallites are thin. For these reasons the absolute crystallinity of wood cannot be determined accurately (Paper III). Most of the studies have aimed at determining the relative crystallinity of wood (Nomura and Yamada, 1972; Tanaka et al., 1981; Dwianto et al., 1996; Kubojima et al., 1997). 15 Both the perpendicular transmission geometry (Fig. 4) and the symmetrical transmission geometry (Fig. 5) have been used for determination of the MFA. In the symmetrical transmission geometry the detector is fixed to the position of the reflection 200 or the reflection 004. If Cu Kα1 radiation (λ = 1.541 Å) is used, the positions of the reflections are 22.6° and 34.6°, respectively. The sample is rotated around its normal and the intensity is measured as a function of the rotation angle φ. This geometry has been used by e.g. Sobue et al. (1971), Lofty et al. (1973), Boyd (1977), Paakkari and Serimaa (1984), and Cave (1997a). In the perpendicular transmission geometry the measurement can be done the same way as in the case of the symmetrical transmission geometry. The detector is fixed to the position of the reflection 200 and then the sample is rotated around its normal and the intensity is measured as a function of the rotation angle φ. There is no need to rotate the sample, if scattered photons are detected using film as was done previously or a two-dimensional detector as is done nowadays. This geometry has been used by Kantola and Seitsonen (1961), Cave (1966), Lofty el al. (1972), Prud’homme et al. (1975), Evans et al. (1996 and 1999), Lichtenegger et al. (1999 and 2003), and Entwistle and Terrill (2000). Figures 11 and 12 show the intensities of the control sample measured in symmetrical and perpendicular transmission mode with the setup described later on in section 7.3. Figure 11 likewise shows the intensities of the cellulose reflection 200 as a function of the rotation angle φ. The intensities are almost identical. Figure 12 presents the intensities of the cellulose reflection 004 as a function of the rotation angle φ. The contributions of the reflection hk3 and hk0 affect the intensity of the reflection 004 (Cave 1997b, Paper I). The use of the reflection 002 does not have this problem, but the cross-section shape of the wood cell also has an effect on the experimental intensity. The intensity of the reflection 004 in the perpendicular transmission mode is too weak to be used for determination of the MFA. Fig. 11 Intensities of the cellulose reflection 200 from a Norway spruce sample from the 14th year ring are measured as a function of the rotation angle φ using both symmetrical transmission and perpendicular transmission geometry. Fig. 12 Intensities of the cellulose reflection 004 from a Norway spruce sample from the 14th year ring are measured as a function of the rotation angle φ using both symmetrical transmission and perpendicular transmission geometry. 16 Small angle x-ray scattering (SAXS) has also been used for determination of MFAs, e.g. Wardrop, 1952; Kantola and Kähkönen, 1963; Kantola et al., 1966; Jakob et al., 1994; Reiterer et al., 1998; Lichtenegger et al., 1999; Entwistle and Terrill, 2000; Entwistle et al. 2005. The results indicate that the SAXS intensity pattern includes one range where scattering from voids dominates and another range where the scattering arises from the electron density contrast between crystalline cellulose and the surrounding material. 5 WAXS measurements 5.1 Microfibril angle The measurements for the determination of the microfibril angle (MFA) were performed using a Siemens θ-2θ diffractometer (Paper I and II). A ground and bent quartz monochromator (the reflection 1110 ) was used to select Cu Kα1 radiation (λ = 1.541 Å). The measurements were performed using the symmetrical transmission mode (Fig. 5). The sample is rotated around its normal and intensity is measured as a function of the rotation angle φ (Fig. 5). The samples were pieces of wood. The scattered photons were detected by a NaI (Tl) scintillation counter. 5.2 Crystallinity The measurements for the determination of the crystallinity of wood were performed using the same diffractometer as the WAXS measurements for MFA (Papers III, IV and V). The diffractometer was used in the symmetrical reflection (Fig. 6) and transmission (Fig. 5) modes. The samples were mainly pieces of wood but a few powdered samples were also studied. The intensity was measured as a function of the scattering angle 2θ by θ-2θ scan. The amorphous background was measured from a sulphate lignin sample. 5.3 The size of cellulose crystallites The measurements for the determination of the size of cellulose crystallites were performed using the same diffractometer as the WAXS measurements for MFA (Paper III). The samples were pieces of wood. The average thickness of cellulose crystallites was determined by measuring the full width at half maximum (FWHM) of the reflection 200 in the pattern measured in the symmetrical reflection mode (Paper III). The thickness of cellulose crystallites was determined from the intensity measured in the reflection mode, because the background is easier to subtract than in the case of the transmission mode. The average length of cellulose crystallites was determined by measuring the FWHM of the reflection 004 in the symmetrical transmission mode (Paper III). Because the samples were tangentially cut, the length of cellulose crystallites could be determined only from the data measured in the transmission mode (compare Figure 9 with Figure 10). The instrumental broadening was 17 obtained from the FWHM of two reflections of a sample of a mixture of lithium fluoride (LiF) and microcrystalline cellulose. The reflections 111 (2θ� 38.8°) and 200 (2θ� 45.1°) of LiF were used. In the case of the reflection 200 the instrumental broadening was 0.21° in 2θ-scale and in the case of the reflection 004 0.30° in 2θ-scale. Because the instrumental broadening was considerable, compared to the FWHM of the reflection 004, the instrumental broadening was reduced by narrower slits. These measurements were done using Huber 420/511 four-circle goniometer (Fig. 13). A ground and bent germanium monochromator (reflection 111) was used to select Cu Kα1 radiation (λ = 1.541 Å). The scattered photons were detected by a NaI (Tl) scintillation counter. Fig. 13 Powder diffractometer. The measurements of the intensity of the reflection 004 were performed using the angular range from 34.0° to 35.5° and the step was 0.02°. The background was assumed to be linear around the reflection 004 and it was determined by measuring the intensity at two angular ranges, in which there are no significant reflections. The angular ranges were from 33.0° to 33.5° and from 36.5° to 37.0° with the step of 0.02°. The divergence slits and the receiving slits were adjusted so that the instrumental broadening would be as small as possible and yet so that detected intensity is reasonable. A sample of a mixture of lithium fluoride (LiF) and microcrystalline cellulose was used. The width of the first divergence slit was 0.2 mm. The second divergence slit and both receiving slits were rectangular, and the width and the height of the slits were 4.0×4.0 mm, 4.0×6.0 mm, and 0.2×6.0 mm, respectively. The instrumental broadening decreased from 0.30° to 0.16° in 2θ- scale. Furthermore, it was studied, whether or not the thickness of the sample had any effect on the FWHM of the reflection 004. Figure 14 presents the intensity curves for the reflection 004 of two Norway spruce samples, which were both taken from the 14th year ring. The thicknesses 18 of the samples were 0.2 mm and 1.0 mm. The values of the FWHM were almost equal but the measuring time of the thinner sample was fivefold longer than the measuring time of the thicker one. Fig. 14 The intensity curve of the reflection 004 of two Norway spruce samples from the 14th year ring. The samples were taken from a stem grown in Asa in southern Sweden. The thickness of the samples was 0.2 mm and 1.0 mm and the FWHM of the reflection 004 was 0.29° and 0.30°, respectively. Measurements were performed using the symmetrical transmission mode. The background was assumed to be linear around the reflection 004 and it was determined by measuring the intensity at two angular ranges, in which there were no significant reflections. The angular ranges were from 33.0° to 33.5° and from 36.5° to 37.0° with a step of 0.02°. 6 Data analysis 6.1 The determination of the microfibril angle The cellulose reflections 200 and 004 are strong enough to be used for the determination of the microfibril angle using the symmetrical transmission mode. The intensity of the reflection 004 immediately reveals the orientation of microfibrils. However, the reflection 004 is overlapped by other reflections (Fig. 12). In the case of the reflection 200, both the orientation of microfibrils and the shape of a cross-section of the cells influence the intensity curve (Cave, 1997a and 1997b). Figure 15 schematically represents one tracheid, which has a rectangular cross-section. The fibre axis is vertical. Two cellulose microfibrils (Z helix) have been drawn, one in the front cell wall and the other in the back cell wall. When the MFA is determined using x-ray scattering and a slice of wood, both the front and back cell wall contribute to the intensity curve (Fig. 15). In order to determine the MFA distribution, the effect of the other cell wall must be eliminated (Fig. 15). 19 Fig. 15 Microfibril angle (MFA) and MFA distribution. The MFA (denoted by α) is the angle between the microfibril and fibre axis. When the intensity curves of the cellulose reflections 200 and 004 have almost the same shape (e.g. Vainio et al., 2002), the MFA distribution is determined from the intensity of the reflection 200. In this case, the shape of a cross-section of the cells is rectangular. When the intensity curve of the reflection 004 has two well separated peaks, and the intensity curve of the reflection 200 has one broad peak with a maximum at a zero angle (e.g. Vainio et al., 2002), the MFA distribution is determined from the intensity of the reflection 004, because the shape of the cross-section of the cells influences the intensity curve of the reflection 200. In this case, the cells have a circular cross-section. Because the MFA distribution of the cell wall is not symmetrical (Peura et al., 2005), it must be modelled as a sum of two or three Gaussian functions. Because both the front and back cell wall contributes to the intensity curve (Fig. 15), a sum of two or three pairs of the Gaussian functions is fitted to the intensity curve. This kind of fitting was made in accordance with Paakkari and Serimaa (1984) and Paper I. The fitting parameters were the positions, the widths and the intensities of the Gaussians and constant background. 6.2 The determination of the crystallinity For determination of the crystallinity, the experimental intensity curve was presented as a linear combination of a calculated diffraction pattern of crystalline cellulose and experimental model intensity for amorphous material in wood. The diffraction pattern of crystalline cellulose was calculated on the basis of the unit cell of Sugiyama et al. (1991). It consisted of fourteen reflections of cellulose, which were presented as Gaussian functions (Fig. 1 of Paper IV). The model was fit to the experimental intensity curve of the wood sample. The fitting parameters included the intensities and the widths of the Gaussians and a scaling factor for the amorphous background. The crystallinity was calculated as a ratio of the integral of the fitted intensity of crystalline cellulose and the integral of the experimental intensity of the wood sample (Paper III). 20 Absolute crystallinities were determined by measuring powdered wood samples by using both symmetrical reflection and symmetrical transmission geometry. The crystallinities were calculated as a weighted mean of crystallinities determined from diffraction patterns measured by the symmetrical reflection and transmission modes. The weights of 31 and 32 for the reflection and transmission data, respectively, were used according to Paakkari et al. (1988). For ensuring that the crystallinity has not diminished during powdering, the average diameter of the crystallites of the powdered samples was also determined and it was observed to be the same as that of the solid oriented samples. The effect of integration limits on the crystallinity were studied by measuring one of the powdered samples at a scattering angle range from 10° to 90° in both reflection and transmission modes. The crystallinity determined from data measured by the reflection mode decreased from 37% to 35% and the crystallinity determined from data measured by the transmission mode increased from 29% to 31% when the upper limit of integration was increased from 50° to 90°. The increase of the upper limit of integration from 50° to 90° did not affect the weighted mean of the crystallinity determined by the transmission and the reflection mode. Therefore, the integration limits were chosen to be from 13° to 50° in agreement with a work by Stubi�ar et al. (1998). 6.3 The determination of the average size of cellulose crystallites The average size of crystallites, Bhkl, was estimated from the widths of the reflections hkl by using the well-known Scherrer formula θθ∆ λ cos2 KB hkl = , where ∆2θ is the FWHM of the reflection in radians and K the shape factor. In the case of the reflection 200, K is supposed to be 0.9. Because the cellulose crystallites are oriented parallel to each other, the shape factor is 1.0 in the case of the reflection 004 (Cullity 1978). The effect of the instrumental broadening on the width of the reflections was included by assuming that the shapes of both the reflection and the instrumental function are Gaussians and the value of ∆2θ was calculated using the formula ∆2θ = (bs2 – bi2)½, where bs is the measured FWHM of the reflection 200 or 004 and bi is the instrumental broadening. The FWHM of the reflection 200 was used in determining the thickness of the cellulose crystallites (Cullity 1978; Papers III, IV and V). Before determining the FWHM of the reflections, the background was subtracted. In the case of the reflection 200, the amorphous background was the same as in determining the crystallinity. In the case of the reflection 004, the background was assumed to be linear. 21 7 Results 7.1 Norway spruce and Scots pine grown in southern Finland Methods to determine the mean microfibril angle (Paper I), the crystallinity of wood (Paper III), and the average size of cellulose crystallites (Paper III and this thesis) were developed. The mean microfibril angle, the crystallinity of wood and the size of cellulose crystallites were determined as a function of the number of the year ring in Norway spruce (Papers II, III and IV) and in Scots pine grown in Finland (Paper III). The mean MFA for Norway spruce is presented as a function of the number of the year ring in Figure 1 of Paper III. The mean MFA close to the pith is over 20° and decreases to about 9° after the 10th year ring. The mean MFA of Scots pine behaves the same way (Paper IV). The average thickness of cellulose crystallites was 32±1 Å (Paper III) and 31±1 Å (these values with the number of the year ring was observed. For Norway spruce the thickness of cellulose crystallites was almost constant as a function of the number of the year ring (Fig. 6 of Paper III). The relative crystallinity for Norway spruce is presented as a function of the number of the year ring in Figure 4 of Paper III. The relative crystallinity increases from the 2nd year ring to 10th year ring and is constant after the 10th year ring. The crystallinity of cellulose for Norway spruce and Scots pine was almost constant as a function of the number of the year ring. The crystallinity of cellulose was 52 ± 3% for both species. The crystallinity of wood and the crystallinity of cellulose behave the same way in Norway spruce and Scots pine (Fig. 3 of Paper IV). 7.2 Irrigated and fertilized Norway spruce grown in southern Sweden The effects of fertilization and irrigation on the cell dimensions of Norway spruce grown in Sweden have been studied earlier (Mäkinen et al., 2002; Lundgren, 2004). In this thesis, it was studied whether fertilization and irrigation influence the length of cellulose crystallites. The lengths of the cellulose crystallites are tabulated in Table 3. The mean length of the cellulose crystallites was 341 Å for irrigated and fertilized samples and 364 Å for the control samples, when the standard deviations were 23 Å and 27 Å, respectively. The difference in the mean values was 23 Å. 22 Sample The number of the year ring FWHM (deg) Length of cellulose crystallites (Å) fertilized 3 0.344 300 mean value: fertilized 4 0.326 320 341 Å fertilized 6 0.311 350 fertilized 8 0.311 340 standard deviation: fertilized 10 0.333 320 23 Å fertilized 14 0.306 350 fertilized 16 0.299 360 fertilized 17 0.291 380 fertilized 18 0.314 340 control 3 0.288 380 mean value: control 4 0.290 380 364 Å control 6 0.317 340 control 8 0.309 350 standard deviation: control 10 0.303 360 27 Å control 14 0.302 360 control 16 0.311 340 control 17 0.269 420 control 18 0.309 350 Table 3. The FWHM of the reflection 004 (FWHM) and the length of the cellulose crystallites (B004) as a function of the number of the year ring for control samples and irrigated and fertilized samples. The mean values of the length of the crystallites in the irrigated and fertilized samples and in the control samples were 341 Å and 364 Å, when the standard deviations were 23 Å and 27 Å, respectively. 7.3 Thermally modified Scots pine grown in Finland In this thesis, it was studied whether thermal modification influences the nanostructure of Scots pine (Paper V). The thermal modification does not influence the MFA distribution (Paper V). The intensity curves as a function of the rotation angle φ for the reflection 200 of a thermally modified sample (230 °C at 4 h) and its reference sample are presented in Figure 16. The MFA distributions of the thermally modified sample and its reference sample are presented in Figure 17. 23 Fig. 16 The intensity I curves as a function of the rotation angle φ for reflection 200 of thermally modified (230 °C at 4 h) sample (solid line) and its reference sample (dots). Fig. 17 The MFA distribution f of thermally modified (230 °C at 4 h) sample (solid line) and its reference sample (dots). The integral �f(φ)dφ = 1, when the integration limits are from -90° to 90°. The thermal modification influences the crystallinity and the thickness of cellulose crystallites of Scots pine wood (Paper V). When the modification temperature is higher than 150 °C, the crystallinity and the diameter of cellulose crystallites increase. When the modification temperature was 230 °C and the time was 4 h, the thickness of the cellulose crystallites increased from 31 Å to 34 Å. Furthermore, it was observed that the reflection 200 shifted to smaller scattering angles as the results of the thermal modification. In this thesis, it was tested whether or not the thermal modification had any influence on the length of cellulose crystallites. Two thermally modified samples (4 h at 180 °C and 4 h at 230 °C) and their reference sample were used in the test measurement. The mean length of the cellulose crystallites for both the thermally modified and the control samples varied between 270 Å and 280 Å. It was not observed that the reflection 004 would have shifted as the reflection 200 had shifted because of the thermal modification. 8 Discussion The mean MFA in Norway spruce decreases rapidly as a function of the number of the year ring and after the 7th year ring it varies between 6° and 10° (Fig. 1a of Paper II). The mean MFA of Scots pine behaves the same way as the mean MFA of Norway spruce (Paper IV). However, the mean MFA of Scots pine is slightly greater than the mean MFA of Norway spruce. Sahlberg et al. (1997) and Lindström et al. (1998) reported similar trends for the MFA of S2 layer. Both groups studied Norway spruce grown in Sweden using WAXS. Sahlberg et al (1997) used symmetrical transmission geometry and Lindström et al. (1998) perpendicular transmission geometry. The values of the mean MFA are in good agreement with the values 24 of Sahlberg et al. (1997). The values of Lindström et al. (1998) are greater than values of Paper II, because they used radial cut samples (Sarén et al., 2004). Lichtenegger et al. (1999) studied Norway spruce and Scots pine grown in Germany using SAXS with perpendicular transmission geometry and assumed the MFA distribution to be Gaussian in the data analysis. Lichtenegger et al. (1999) reported similar trends for the MFA of S2 layer of both species but the values for Norway spruce were smaller than values in Paper II and the values for Scots pine were larger than values in Paper IV. They reported even values of zero degrees for Norway spruce, which results from the use of a poor fitting model. According to Paper II there is a connection between the mean MFA and the tracheid diameter and length. The mean MFA decreased and the diameter of the tracheid increased rapidly roughly up to the 10th year ring and did not change much after that toward the bark. The tracheid length increased also rapidly towards the bark. Furthermore, the cross-sectional shape of the tracheid is hexagonal near the pith and becomes rectangular toward the bark (Paper II). The thickness of cellulose crystallites for Norway spruce appears to be constant as a function of the number of the year ring (Fig. 6 of Paper III). The thickness was about 32 Å for the whole studied year ring range, from the 2nd year ring to the 42nd year ring, (Papers III and IV). Marton et al. (1972) observed similar behaviour for Norway spruce grown in Syracuse (New York, USA). The thicknesses varied between 30 Å and 35 Å. In Paper I a slightly smaller value of 29 Å was obtained for compression wood of Norway spruce. Marton et al. (1972) also observed that the thickness in compression wood is smaller than that of normal wood. On the other hand, the thickness in tension wood is greater than the thickness in the normal wood (Marton et al., 1972; Washusen and Evans, 2001). Washusen and Evans (2001) studied Eucalyptus globulus and observed that the thickness of cellulose crystallites is 36 Å in tension wood and 32 Å in normal wood. The thickness of cellulose crystallites for Scots pine was about 31 Å (Paper IV). Nomura and Yamada (1972) and Tanaka et al. (1981) have reported values of 28-32 Å for another pine species, Pinus densiflora. Thus, the value of 32 Å for Norway spruce and 31 Å for Scots pine are in accord with the values reported previously. The result that the cellulose crystallites have the same thickness from the pith to the bark may indicate that the cellulose synthesis occurs the same way in every year ring in both Norway spruce and Scots pine. The spacing 200d of the cellulose I structure is 3.867 Å (Nishiyama et al., 2002). The thickness of cellulose crystallites is about 32 Å indicating that the cross-section of cellulose crystallite consists on average of 4×4 unit cells (Fig. 18). Then the cellulose crystallite would consist of 32 cellulose chains. On the other hand, it has been proposed that the rosette consists of 36 CESAs, each of which polymerises glucose molecules into cellulose chains (Cosgrove, 2005). On this basis, the thickness of cellulose crystallites is reasonable. 25 Fig. 18 The cross-section of cellulose crystallite from the direction [001]. Because the thickness of cellulose crystallite was 31-32 Å, the cross-section may consist of 4 × 4 unit cells of the cellulose I and 32 cellulose chains. The crystallinity of cellulose in Norway spruce and Scots pine was constant (52%) as a function of the year ring (Paper IV). Leary et al. (1987) reported, using NMR spectroscopy, that the crystallinity of cellulose for Pinus radiata is smaller in heartwood than in mature wood. Newman and Hemmingson (1990) obtained a greater value of 62% for Norway spruce but their value of 54% for Pinus radiata agrees with the values of Paper IV for Scots pine. Fig. 19. The schematic model of the cellulose microfibril. On the surface of the cellulose crystallites there is a 2 Å thick layer of amorphous cellulose. If the crystallinity of cellulose is 52%, there should be 189 Å long amorphous regions between two consecutive crystalline regions of the cellulose microfibrils. Figure 19 shows a schematic model of the cellulose microfibril drawn on the basis of the WAXS results. Here, it was supposed for simplicity that all cellulose is in the form of microfibrils. The estimation that there is a 2 Å thick layer of amorphous cellulose at the surface of the cellulose crystallites (Fig. 19) is based on the TEM studies of Donaldson and Singh (Donaldson and Singh, 1998), according to which the average diameter of cellulose microfibrils is 36 Å; moreover, this is also based on the results of Paper III, according to 26 which the diameter of cellulose crystallites is 32 Å. The length of the crystalline regions is ascertained to be 364 Å. If the crystallinity of cellulose is 52% and all cellulose is in the microfibrils, there should be 189 Å long amorphous regions between crystalline regions of the cellulose microfibrils. The mass fraction of crystalline cellulose in the cell wall increases with both the ring number and distance from the pith (Papers III and IV). Marton et al (1972) observed a similar dependence between the crystallinity index and the number of the year ring. The thickness of cellulose crystallites (Papers III and IV) and the crystallinity of cellulose (Paper IV) were constant as a function of the number of the year ring. Therefore, the increase in crystallinity of wood must be due to a decreased lignin and hemicellulose content as a function of the number of the year ring (Panshin and de Zeeuw, 1980; Bertaud and Holmbom, 2004). The mass fraction of cellulose in wood was calculated from the crystallinity of wood and the crystallinity of cellulose (Paper IV). It increased with the distance from the pith from 44% to 58% for Norway spruce and from 47% to 62% for Scots pine (Paper IV). The accuracy of the values was estimated to be 10%. For the mass fraction of cellulose in Norway spruce Fengel and Wegener (1984) give a value of 46% and Sjöström (1993) gives a value of 41.7%. According to Anttonen et al. (2002), the mass fraction of cellulose in Norway spruce is 48%. For Scots pine, Fengel and Wegener (1984) give a fraction of 52% and Sjöström (1993) gives a fraction of 40.0%. So, the calculated mass fractions of cellulose for Norway spruce and Scots pine are in accord with these literature values. The good agreement indicates that using powdered wood samples, and by correcting the results for fibre texture, it is possible to estimate the crystallinity of wood by WAXS, although wood is a complex material. Because of the fibre texture, the relative crystallinity values of the solid wood samples, determined by the reflection mode, are clearly too high compared to the crystallinity values determined from the powdered samples, but these relative crystallinity values are correlated with the crystallinities determined using powdered samples (Paper III). If a set of solid oriented samples has the same kind of fibre texture, the relative crystallinity values determined using solid oriented samples could be used. Amorphous materials, like hemicellulose, degrade as a result of the thermal modification (Wikberg and Maunu, 2004). This is one reason for the increase of the crystallinity of wood due to the modification temperature. The other reason is the increase of the crystallinity of cellulose (Sivonen et al., 2002). When the modification temperature exceeds 180 ºC, the decrease in the FWHM of the reflection 002 corresponds to an approximate 3 Å increase in the thickness of the crystallites (Fig. 2 of Paper V). Obviously, this change is mainly due to the release of strains and a decrease in the amount of defects in cellulose crystallites (Goring, 1963). The increase of the thickness of the crystallites is consistent with the increase of crystallinity of cellulose due to the thermal modification (Sivonen et al., 2002). The reflection 200 was shifted to smaller scattering angles due to the thermal modification. Hori and Wada (2005) observed shifting of the same kind, when they studied the thermal expansion of wood cellulose crystallites in tension wood (Populus maximowiczii) from room temperature to 250 ºC. They observed that the equatorial d-spacings, 011d , 110d , and 200d , increased dramatically above 180 ºC. Hori and Wada (2005) proposed that cellulose is transformed into a high-temperature phase. On the other hand, the intrinsic stresses in wood 27 can also release and so it is easier for the crystallites to expand when the temperature increases. Unfortunately, Hori and Wada (2005) did not report on how these d-spacings behave, when the temperature decreases back to room temperature. The observation that the reflection 004 did not shift due to the thermal modification is consistent with the observation of Hori and Wada (2005). Fig. 20 A SEM image of transverse section of earlywood tracheids in a thermally modified (4 h at 230 ºC) Scots pine sample. (Courtesy of Tuuli Timonen and Pirkko Harju, Botanical Museum, Univ. of Helsinki) Fig. 21 A SEM image of transverse section of earlywood tracheids in a reference Scots pine sample. (Courtesy of Tuuli Timonen and Pirkko Harju, Botanical Museum, Univ. of Helsinki) The MFA distributions for thermally modified and reference samples were almost equal (Fig. 17). It is interesting to observe that the thermal modification did not markedly affect the MFA distribution. Figure 20 presents a scanning electron microscopy (SEM) image of the transverse section of earlywood tracheids in a thermally modified (4 h at 230 ºC) Scots pine sample and Figure 21 presents a corresponding SEM image from its reference sample. When Figures 20 and 21 are compared with each other, one can observe that the thermal modification does not change the micrometer level anatomical structure of wood. Thus, it is difficult to imagine a situation in which the cellulose microfibrils could turn inside the cell wall so that the MFA distribution would change notably. However, a single cellulose crystallite in the cellulose microfibril could turn to a certain direction, but its neighbouring cellulose crystallite should turn simultaneously to the opposite direction. In this case, the mean MFA would not change but the standard deviation of the MFA distribution could increase slightly. Because the MOE of crystalline cellulose is greater than the MOE of amorphous cellulose (e.g. Salmén and de Ruvo, 1985; Bergander and Salmén, 2002), the MOE of cellulose increases with the increasing crystallinity of cellulose. Although the crystallinity of wood increases as a function of the modification temperature (Paper V), the longitudinal MOE of 28 wood decreases as a function of the modification temperature (Hæggström et al., 2005). There was no clear correlation between the crystallinity of wood and the MOE. The reason for the decrease of MOE could be the weakening of the amorphous matrix. However, Hæggström et al. (2005) used samples, which contain both earlywood and latewood, and in the crystallinity measurements only earlywood samples were used. According to Table 3, fertilization and irrigation affect the length of cellulose crystallites for Norway spruce. This indicates that the growth rate may influence the length of cellulose crystallites. However, further studies are needed to clarify this. It would also be interesting to study whether fertilization and increased growth rate influence crystallinity of wood and cellulose and the thickness of cellulose crystallites. Fertilisation and irrigation increased the growth rate and resulted in much thinner cell walls than untreated control trees (Mäkinen et al., 2002). 9 Conclusions The reliability of x-ray scattering methods to study the nanostructure of the wood cell wall was evaluated and reliable measurement and data analysis procedures were developed. For determination of the orientation of microfibrils, the symmetrical transmission geometry seems to be better than the perpendicular transmission geometry (Paper II). Using the symmetrical transmission geometry it is possible to obtain information on both the orientation of microfibrils and the shape of the cross-section of the cells. Using powdered samples and both the reflection and transmission geometry the crystallinity of wood could be reliably determined. These methods were used to study the nanostructure of Norway spruce and Scots pine. The mean MFA decreases rapidly from the pith to the bark and after the 7th year ring it varies between 6º and 10º. The crystallinity of wood increases from the 2nd year ring to the 10th year ring 10 and is constant after the 10th year ring. The crystallinity of cellulose obtained using nuclear magnetic resonance spectroscopy was 52% for both species. The nanostructure does not account for the small differences between longitudinal MOE of Norway spruce and Scots pine (Table 1). However, these differences can be explained by the differences on the tissue level. For instance, the length of the tracheids and the thickness of the cell wall for Norway spruce and Scots pine differ slightly from each other. The thermal modification increases the crystallinity of wood and the thickness of cellulose crystallites. This result is consistent with the reported increase of the crystallinity of cellulose in thermally modified Scots pine (Sivonen et al. 2002). The increase of the crystallinity of wood is in accord with the observation, that the thermally modified wood is more brittle than untreated wood. It would be interesting to study how the modification temperature influences the thermal expansion of the cellulose crystallites. The bonding of surface chains of cellulose microfibrils to the other cell wall components may cause lattice distortions in cellulose microfibrils. On this basis, it would be interesting to study how the mass fractions of cell wall components influence the thickness and length of cellulose crystallites. The chain termination and initiation during cellulose synthesis may also cause 29 lattice distortions. Because growth rate may affect the frequency of chain terminations, it would be interesting to study whether, and to what extent, the growth rate influences the dimensions of cellulose crystallites. Besides determining the thickness and length of cellulose crystallites using WAXS, it would be possible to also determine the distance between cellulose microfibrils using SAXS. The results could thus give new information on the formation mechanism of the cell wall. 10 References Abe H., Ohtani J., Fukazawa K. (1991) FE-SEM observations on the microfibrillar orientation in the secondary wall of tracheids. IAWA Bulletin n.s. 12 (4): 431-438. Alexander, L. E. (1969) X-ray Diffraction Methods in Polymer Science. John Wileys & Sons, Inc., New York, USA, pp. 137-197. Anttonen S., Manninen A.-M., Saranpää P., Kainulainen P., Linder S., Vapaavuori E. (2002) Effects of long-term nutrient optimisation on stem wood chemistry in Picea abies. Trees - Structure and Function 16 (6): 386-394. Astley R.J., Stol K.A., Harrington J.J. (1998) Modelling the elastic properties of softwood - Part II: The cellular microstructure. Holz als Roh- und Werkstoff 56 (1): 43-50. Atalla R.H., VanderHart D.L. (1984) Native Cellulose: A composite of two distinct crystalline forms. Science 223 (4633): 283-284. Balta-Calleja, F.J., and Vonk, C.G. (1989) X-ray scattering of synthetic polymers. Elsevier, Amsterdam, Holland, pp. 175-204. Bernatzky A. (1978) Developments in agricultural and managed- Forest ecology, 2 Tree ecology and preservation. Elsevier Scientific Publishing Company, Amsterdam, The Netherlands. Bergander A., Salmén L. (2002) Cell wall properties and their effects on the mechanical properties of fibers. Journal of Materials Science 37 (1): 151-156. Bertaud F., Holmbom B. (2004) Chemical composition of earlywood and latewood in Norway spruce heartwood, sapwood and transition zone wood. Wood Science and Technology 38 (4): 245-256. Boyd J.D. (1977) Interpretation of x-ray diffractograms of wood for assessments of microfibril angles in fibre cell walls. Wood Science and Technology 11 (2): 93-114. Cave I.D. (1966) Theory of x-ray measurement of microfibril angle in wood. Forest Products Journal 16 (10): 37-42. Cave I.D. (1997a) Theory of x-ray measurement of microfibril angle in wood. Part 1. The condition for reflection. X-ray diffraction by materials with fibre type symmetry. Wood Science and Technology 31 (3): 143-152. 30 Cave I.D. (1997b) Theory of x-ray measurement of microfibril angle in wood. Part 2. The diffraction diagram. X-ray diffraction by materials with fibre type symmetry. Wood Science and Technology 31 (4): 225-234. Cave I.D., Walker J.C.F. (1994) Stiffness of wood in fast-grown plantation softwoods: The influence of microfibril angle. Forest Products Journal 44 (5): 43-48. Cosgrove D.J. (2005) Growth of the plant cell wall. Nature Reviews Molecular Cell Biology 6 (11): 850-861. Cullity B.D. (1978) Elements of x-ray diffraction. 2nd edition Addison-Wesley Publishing company, Inc. Reading, Massachusetts, USA, pp. 100-102. Donaldson L.A. (1991) The use of pit apertures as windows to measure microfibril angle in chemical pulp fibers. Wood and Fiber Science 23 (2): 290-295. Donaldson L.A., Singh A.P. (1998) Bridge-like structures between cellulose microfibrils in radiata pine (Pinus radiata D. Don) kraft pulp and holocellulose. Holzforschung 52 (5): 449- 454. Dwianto W., Tanaka F., Inoue M., Norimoto M. (1996) Crystallinity changes of wood by heat or steam treatment. Wood Research 83: 47-49. Evans R., Stuart S.-A., Van der Touw J. (1996) Microfibril angle scanning of increment cores by x-ray diffractometry. Appita Journal 49 (6): 411-414. Evans R., Hughes M., Menz D. (1999) Microfibril angle variation by scanning x-ray diffractometry. Appita Journal 52 (5): 363-367. Entwistle K.M., Terrill N.J. (2000) The measurement of the micro-fibril angle in soft-wood. Journal of Materials Science 35 (7): 1675-1684. Entwistle K.M., Eichhorn S.J., Navaranjan N. (2005) The derivation of the cellulose microfibril angle by small-angle x-ray scattering from structurally characterized softwood cell-wall populations. Journal of Applied Crystallography 38: 505-511. Fagerstedt K., Pellinen K., Saranpää P., Timonen T. (1996) Mikä puu - mistä puusta. Yliopistopaino, Helsinki, Finland, pp. 20-21. Fengel D., Wegener G. (1984) Wood chemistry, ultrastructure, reactions. Walter de Gruyter, Berlin, Germany. Fries A., Ericsson T., Mörling T. (2003) Measuring relative fibre length in Scots pine by non- destructive wood sampling. Holzforschung 57 (4): 400-406. Goring D.A.I. (1963) Thermal softening of lignin, hemicellulose and cellulose. Pulp and Paper Magazine of Canada 64: T517-T527. Hakkila P. (1966) Investigations on the basic density of Finnish pine, spruce and birch wood. Communicationes Instituti Forestalis Fenniae 61 (5): 1-98. 31 Harrington J.J., Booker R., Astley R.J. (1998) Modelling the elastic properties of softwood. Part I: The cell-wall lamellae. Holz als Roh- und Werkstoff 56 (1): 37-41. Hori R., Wada M. (2005) The thermal expansion of wood cellulose crystals. Cellulose 12 (5): 479-484. Hæggström E., Wallin A., Hoffren H., Hassinen T., Viitaniemi P. (2005) Study on attenuation, modulus of elasticity and nonlinearity in thermowood using ultrasound. AIP- Conference-Proceedings 760: 1500-1506. Inagaki H. (1989) Historical survey of cellulose research in Japan. In: Kennedy, J.F., Phillips G.O., Williams P.A. (editors) Cellulose structural and functional aspects, Ellis Horwood limited, Southampton, Great Britain. pp. 3-17. Jakob H.F., Fratzl P., Tschegg S.E. (1994) Size and arrangement of elementary cellulose fibrils in wood cells: A small-angle x-ray scattering study of Picea abies. Journal of Structural Biology 113 (1): 13-22. Jakob H.F., Fengel D., Tschegg S.E., Fratzl P. (1995) The elementary cellulose fibril in Picea abies: Comparison of transmission electron microscopy, small-angle x-ray scattering, and wide-angle x-ray scattering results. Macromolecules 28 (26): 8782-8787. Kantola M., Seitsonen S. (1961) X-ray orientation investigations on Finnish conifers. Annales Academiæ Scientiarum Fennicæ. Series A VI Physica 80: 1-15. Kantola M., Kähkönen H. (1963) Small-angle x-ray investigation of the orientation of crystallites in Finnish coniferous and deciduous wood fibers. Annales Academiæ Scientiarum Fennicæ. Series A VI Physica 137: 1-14. Kantola M., Kähkönen H., Seitsonen S. (1966) On the correspondence of the small-angle and wide-angle x-ray diffraction patterns of wood fibers. Annales Academiæ Scientiarum Fennicæ. Series A VI Physica 220: 1-9. Kantola M., Seitsonen S. (1969) On the relation between tracheid length and microfibrillar orientation measured by x-ray diffraction in conifer wood. Annales Academiæ Scientiarum Fennicæ. Series A VI Physica 300: 1-10. Keckes J., Burgert I., Frühmann K., Müller M., Kölln K., Hamilton M., Burghammer M., Roth S.V., Stanzl-Tschegg S., Fratzl P. (2003) Cell-wall recovery after irreversible deformation of wood. Nature Materials 2 (12): 810-814. Kennedy R.W. (1995) Coniferous wood quality in the future: Concerns and strategies. Wood Science and Technology 29 (5): 321-338. Koponen S., Toratti T., Kaneva P. (1989) Modelling longitudinal elastic and shrinkage properties of wood. Wood Science and Technology 23 (1): 55-63. Koponen S., Toratti T., Kaneva P. (1991) Modelling elastic and shrinkage properties of wood based on cell structure. Wood Science and Technology 25 (1): 25-32. 32 Koponen T., Karppinen T., Hæggström E., Saranpää P., Serimaa R. (2005) The stiffness modulus in Norway spruce as a function of year ring. Holzforschung 59 (4): 451-455. Kubojima Y., Okano T., Ohta M. (1997) Effect of annual ring widths on structural and vibrational properties of wood. Mokuzai Gakkaishi 43 (8): 634-641. Leney L. (1981) A technique for measuring fibril angle using polarized light. Wood and Fiber 13 (1): 13-16. Leary G.J., Morgan K.R., Newman R.H. (1987) Solid state carbon-13 nuclear magnetic resonance study of Pinus radiata wood. Appita Journal 40 (3): 181-184. Lichtenegger H., Reiterer A., Stanzl-Tschegg S.E., Fratzl P. (1999) Variation of cellulose microfibril angles in softwoods and hardwoods. - A possible strategy of mechanical optimazation. Journal of Structural Biology 128 (3): 257-269. Lichtenegger H.C., Müller M., Wimmer R., Fratzl P. (2003) Microfibril angles inside and outside crossfields of Norway spruce tracheids. Holzforschung 57 (1): 13-20. Lindström H. (1997) Fiber length, tracheid diameter, and latewood percentage in Norway spruce: Development from pith outwards. Wood and Fiber Science 29 (1): 21-34. Lindström H., Evans J.W., Verrill S.P. (1998) Influence of cambial age and growth conditions on microfibril angle in young Norway spruce (Picea abies [L.] Karst.). Holzforschung 52 (6): 573-581. Lofty M., El-osta M., Wellwood R.W., Butters R.G. (1972) An improved x-ray technique for measuring microfibril angle of coniferous wood. Wood Science 5 (2): 113-117. Lofty M., El-osta M., Kellogg R.M., Foschi R.O., Butters R.G. (1973) A direct x-ray technique for measuring microfibril angle. Wood and Fiber 5 (2): 118-128. Lundgren C. (2003) Wood and fibre properties of fertilized Norway spruce. Doctor’s dissertation Acta Universitatis agriculturae Sueciae. Silvestria vol. 288. Lundgren C. (2004) Cell wall thickness and tangential and radial cell diameter of fertilized and irrigated Norway spruce. Silva Fennica 38 (1): 95-106. Marton R., Rushton P., Sacco J.S., Sumiya K. (1972) Dimensions and ultrastructure in growing fibers. Tappi 55 (10): 1499-1504. Mauseth J.D. (2003) Botany: an introduction to plant biology. 3rd ed. Jones and Bartlett Publishers, Boston, USA. Meyer K.H., Misch L. (1937) Positions des atomes dans le nouveau modèle spatial de la cellulose. Helvetica Chimica Acta 20: 232-244. Mäkinen H., Saranpää P., Linder S. (2002) Effect of growth rate on fibre characteristics in Norway spruce (Picea abies (L.) Karst.). Holzforschung 56 (5): 449-460. 33 Newman R.H., Hemmingson J.A. (1990) Determination of the degree of cellulose crystallinity in wood by carbon-13 nuclear magnetic resonance spectroscopy. Holzforschung 44 (5): 351-355. Nishiyama Y., Langan P., Chanzy H. (2002) Crystal structure and hydrogen-bonding system in cellulose I from synchrotron x-ray and neutron fiber diffraction. Journal of the American Chemical Society 124 (31): 9074-9082. Nishiyama Y., Sugiyama J., Chanzy H., Langan P. (2003) Crystal structure and hydrogen bonding system in cellulose I. from synchrotron x-ray and neutron fiber diffraction. Journal of the American Chemical Society 125 (47): 14300-14306. Nobel P.S. (1999) Physicochemical and environmental plant physiology. 2nd edition. Academic Press, San Diego, USA. Nomura T., Yamada T. (1972) Structural observation on wood and bamboo by x-ray. Wood Research 52: 1-12. Nuopponen M., Vuorinen T., Jämsä S., Viitaniemi P. (2003) The effects of a heat treatment on the behaviour of extractives in softwood studied by FTIR spectroscopic methods. Wood Science and Technology 37 (2): 109-115. Paakkari T., Serimaa R. (1984) A study of the structure of wood cells by x-ray diffraction. Wood Science and Technology 18 (2): 79-85. Paakkari T., Blomberg M., Serimaa R., Järvinen M. (1988) A texture correction for quantitative x-ray powder diffraction analysis of cellulose. Journal of Applied Crystallography 21 (5): 393-397. Panshin A.J., de Zeeuw C. (1980) Textbook of wood technology: Structure, identification, properties, and uses of the commercial woods of the United States and Canada, 4th edition. McGraw-Hill, New York, USA. Peura M., Müller M., Serimaa R., Vainio U., Sarén M.-P., Saranpää P., Burghammer M. (2005) Structural studies of single wood cell walls by synchrotron x-ray microdiffraction and polarised light microscopy. Nuclear Instruments and Methods in Physics Research B 238: 16- 20. Prud’homme R.E., Noah J. (1975) Determination of fibril angle distribution in wood fibers: A comparison between the x-ray diffraction and the polarized microscope methods. Wood and Fiber 6 (4): 282-289. Reiterer A., Jakob H.F., Stanzl-Tschegg S.E., Fratzl P. (1998) Spiral angle of elementary cellulose fibrils in cell walls of Picea abies determined by small-angle x-ray scattering. Wood Science and Technology 32 (5): 335-345. Ruland W. (1961) X-ray determination of crystallinity and diffuse disorder scattering. Acta Crystallographica 14 (11): 1180-1185. 34 Sahlberg U., Salmén L., Oscarsson A. (1997) The fibrillar orientation in the S2-layer of wood fibres as determined by x-ray diffraction analysis. Wood Science and Technology 31 (2): 77- 86. Salmén L., de Ruvo A. (1985) A model for the prediction of fiber elasticity. Wood and Fiber Science 17 (3): 336-350. Saranpää P. (1994) Basic density, longitudinal shrinkage and tracheid length of juvenile wood of Picea abies (L.) Karst. Scandinavian Journal of Forest Research 9 (1): 68-74. Saranpää P., Serimaa R., Andersson S., Pesonen E., Suni T., Paakkari T. (1998) Variation of microfibril angle of Norway spruce (Pinus abies (L.) Karst.) and Scots pine (Pinus sylvestris L.) – comparing x-ray diffraction and optical methods. In: Butterfield BG (editor) Microfibril angle in wood. Christchurch: University of Canterbury, New Zealand, pp. 240-252. Sarén M.-P., Serimaa R., Andersson S., Saranpää P., Keckes J., Fratzl P. (2004) Effect of growth rate on mean microfibril angle and cross-sectional shape of tracheids of Norway spruce. Trees -Structure and Function 18 (3): 354-362. Singh A.P., Daniel G. (2001) The S2 layer in the tracheid walls of Picea abies wood: Inhomogeneity in lignin distribution and cell wall microstructure. Holzforschung 55 (4): 373- 378. Sisson W.A. (1935) X-ray studies of crystallite orientation in cellulose fibers. Natural fibers. Industrial and Engineering Chemistry 27 (1): 51-56. Sivonen H., Maunu S.L., Sundholm F., Jämsä S., Viitaniemi P. (2002) Magnetic resonance studies of thermally modified wood. Holzforschung 56 (6): 648-654. Sjöström E., (1993) Wood chemistry. Fundamentals and applications, 2nd edition. Academic Press, San Diego, USA. Sobue N., Hirai N., Asano I. (1971) Studies on structure of wood by x-ray. II. Estimation of the orientation of micells in cell wall. Mokuzai Gakkaishi 17 (2): 44-50. Stubi�ar N., Šmit I., Stubi�ar M., Tonejc A., Jánosi A., Schurz J., Zipper P. (1998) An x-ray diffraction study of the crystalline to amorphous phase change in cellulose during high-energy dry ball milling. Holzforschung 52 (5): 455-458. Sugiyama J., Vuong R., Chanzy H. (1991) Electron diffraction study on the two crystalline phases occuring in native cellulose from an algal cell wall. Macromolecules 24 (14): 4168- 4175. Tanaka F., Koshijima T., Okamura K. (1981) Characterization of cellulose in compression and opposite woods of a Pinus densiflora tree grown under the influence of strong wind. Wood Science and Technology 15 (4): 265-273. Tang R.C. (1973) The microfibrillar orientation in cell-wall layers of Virginia pine tracheids. Wood Science 5 (3): 181-186. 35 Vainio U., Andersson S., Serimaa R., Paakkari T., Saranpää P., Treacy M., Evertsen J. (2002) Variation of microfibril angle between four provenances of Sitka spruce (Picea sitchensis [Bong.] Carr.). Plant Biology 4 (1): 27-33. Vainio U., Maximova N., Hortling B., Laine J., Stenius P., Simola L.K., Gravitis J., Serimaa R. (2004) Morphology of dry lignins and size and shape of dissolved kraft lignin particles by x-ray scattering. Langmuir 20 (22): 9736-9744. Verkasalo E., Leban J.-M. (2002) MOE and MOR in static bending of small clear specimens of Scots pine, Norway spruce and European fir from Finland and France and their prediction for the comparison of wood quality. Paperi ja Puu - Paper and Timber 84 (5): 332-340. Viitaniemi P., Jämsä S., Ek P., Viitanen H. (1994) Pat. US-5678324 Method for improving biodegradation resistance and dimensional stability of cellulosic products. Appl. 545791 , 13.5.1994. Publ. 24.11.1994. 12p. Viitaniemi P., Jämsä S., Ek P. (1995) Pat. FI 103834, Menetelmä puun kuivaamiseksi. Appl. 942210, 11.05.1994. Publ. 12.11.1995. 6p. Vonk C.G. (1973) Computerization of Ruland’s x-ray method for determination of the crystallinity in polymers. Journal of Applied Crystallography 6 (APR1): 148-152. Vonk C.G., Fagherazzi G. (1983) The determination of the crystallinity in glass-ceramic materials by the method of Ruland. Journal of Applied Crystallography 16 (APR): 274-276. Wagenführ R., Scheiber Chr. (1989) Holzatlas. Mit 890 zum Teil Mehrfarbigen Bildern. 3. Auflage. VEB Fachbuchverlag, Leipzig, GDR, pp. 656, 665. Wardrop A.B. (1952) The low-angle scattering of x-rays by conifer tracheids. Textile Research Journal 22 (4): 288-291 Washusen R., Evans R. (2001) The association between cellulose crystallite width and tension wood occurrence in Eucalyptus globules. IAWA Journal 22 (3): 235-243. Wikberg H., Maunu S.L. (2004) Characterisation of thermally modified hard- and softwoods by 13C CPMAS NMR. Carbohydrate Polymers 58 (4): 461-466.